Zirconium  Processing
Serial NumberTechnologyProcess Description
1ingot casting inspectioncomposition reinspection, appearance inspection
2β forgingheated in furnace under temperature of 1030-1050˚C, insulated for 60 to 90 min, water quenching

3drilling, boring, copper lad set
4extrudingline frequency induction furnace heat to 750-780˚C, insulated for 30 to 35 min, extruding on 3150t extruding machine
5tube billets repair
6cold rolling and intermediate annealing rolling after 3-4 times, intermediate annealing at 700˚C, insulated for 1h, vacuum degree 10-2Pa-10-3Pa
7precision rollingprecision rolling after 3-4 times. General working rate over 70%, Q data is 3-5
8finishing annealingrecrystallization annealing: 545+/-5˚C, insulated 2h. stress relief annealing: 460+/-5˚C, insulated 3h
9straighteningon roller leveler
10inner surface acid washuse flowing acid
11outer surface polishinguse abrasive belt
12dimension inspection
13property inspection
14packing